0

ASTM D7078 - V-Notched Rail Shear Testing Method of CFRP

  • ASTM D7078 (Standard Test Method for Shear Properties of Composite Materials by V-Notched Rail Shear Method) is a V-notched rail shear testing method that is widely used to determine the in-plane shear characteristics of composite materials. This method uses a sample without holes with a large gauge section and can accommodate CFRPs with discontinuous fibers.

    Shear strain can be calculated using the AGX Series, TRAPEZIUM X Series software and an ASTM D7078 test jig. For this test, two strain gauges were attached at the midpoint between the V notches in order to measure strain in -45° and +45° directions. The equipment configuration is shown in Table 1. Table 2 shows that the test results are highly reproducible.

  • Table 1: ASTM D7078 Test Conditions

    Testing Machine AGX Series
    Load Cell 50 kN
    Test Jig ASTM D7078 Jig
    Software TRAPEZIUM X Series (Single)
    Test Speed 2 mm/min
  • Table 2: ASTM D7078 Test Results

    Specimen Shear Modulus
    (GPa)
    Shear Strength
    (MPa)
    Test 1 4.63 121.72
    Test 2 4.55 120.00
    Test 3 4.58 120.05
    Mean 4.59 120.60
  • ASTM D7078 Specimen Shear Strain Distribution

    ASTM D7078 Shear Strain Distribution
  • ASTM D7078 Specimen After Testing

    ASTM D7078 Test Specimen

Recommended Products for ASTM D7078